Cold shunt and misrun casting, Other Engineering

Q. Discuss briefly the causes and remedies of misrun and cold shunts casting  

Cold Shunt and Misrun : When the metal is unable to fill the     mould cavity completely and thus leaving unfilled portion called misrun. A cold shunt is called when two metal streams do not fuse together properly.

       Causes : (i) Lake of fluidity in molten metal

                 (ii) Faulty design               (iii) Faulty gating

       Remedies : (i) Adjust proper pouring temperature

                 (ii) Modify design              (iii) Modify gating system

Posted Date: 8/3/2012 2:24:40 AM | Location : United States







Related Discussions:- Cold shunt and misrun casting, Assignment Help, Ask Question on Cold shunt and misrun casting, Get Answer, Expert's Help, Cold shunt and misrun casting Discussions

Write discussion on Cold shunt and misrun casting
Your posts are moderated
Related Questions
Each student will, as part of the course requirements, submit a research paper on an individual stock. You are allowed to select any stock that trades on the New York Stock Exchang

the requirements are 1- prescriptive analysis of occupancy through prescriptive code analysis with in- depth information related to the egress.2- fire scenario design realistic and

The firm is considering an investment opportunity. The investment falls in the same class of risk as the firm, the project is financed with equity and debt. Explain all the steps i

list out the errors in lenier measurment

et C(K) denote a European vanilla Call option with strike price K. Assume that all options are identical except for strike price, and strike prices satisfy (K1) What are the no-a

FLIGHT FINE PITCH STOP FAILURE (OVERSPEED) An overspeed is prevented by an automatic coarsening device. A switch mounted on the Hub closes when the blade angle is below Flig

Q. 1 A 50 cm diameter pipeline in the Arctic Carries hot oil at 30 0C and exposed to a coefficient surrounding temperature of -20 0C. Special powder insulation 5 cm thick surround

The oil pressure indicator : The oil pressure indicator has a dial normally calibrated in pounds per square inch (psi). The indicator may have max. limit markers, but will alw

Shelf List Filing   Shelf list reflects the arrangement of documents in the library. That is to say, the classificatory arrangement of the documents in a library can be seen th

Plasma Arc Welding (PAW) is a special form of gas tungsten arc welding in which constricted plasma arc is directed at the weld area. In PAW, a tungsten electrode is contained in a